Splay (silver streaks): moisture, gas or air? How to separate the cause and the order of fixes
Silvery streaks running in the flow direction usually come from moisture, but that is not the only cause. Diagnosis with an air shot, allowed moisture by material, the order of adjustments and the causes on the mold side.

Splay (silver streaks) are silvery or whitish streaks on the part surface running in the flow direction. Small gas bubbles in the melt reach the flow front, burst and stretch when they touch the mold wall, and leave a mark on the surface. So behind every silver streak there is gas. The task is to find where that gas comes from. There are three main sources: moisture, volatiles from thermal degradation and air trapped in the screw or the mold.
First step: the air shot
With the mold open, retract the nozzle, inject a few shots into the air and look at the melt.
- Foamy melt, crackling, steam coming out: almost certainly moisture. Check drying first.
- Darker or yellowed melt with a sharp smell: thermal degradation. Temperature or residence time is too high.
- Clean, glossy melt but the part still has streaks: the gas most likely comes from air drawn in during plasticizing or from the mold side.
This three-minute test often saves hours of wrong adjustments.
Moisture: the most common cause
Hygroscopic materials draw moisture from the air into the pellet. At melt temperature this moisture turns into steam. A hot-air dryer that only heats the surface is not enough for these materials; a desiccant (dry-air) dryer is needed.
Common upper limits (the material supplier's data sheet takes priority):
| Material | Allowed moisture (approx.) |
|---|---|
| PC | ≤ 0.02% |
| PBT | ≤ 0.02–0.04% |
| PET | ≤ 0.005% (50 ppm) |
| PA6 / PA66 | ≤ 0.1–0.2% |
| ABS | ≤ 0.1% |
| PMMA | ≤ 0.05–0.1% |
The most frequent drying mistakes:
- Not time, but airflow and dew point: even if the dryer shows the right temperature, the material is not dry enough if the dew point is above −30 °C or the hopper is too small for the hourly throughput.
- Dry material picking up moisture again: a long, open conveying line or an open feed hopper between dryer and machine undoes the drying.
- Over-drying: with materials such as PA, drying too long or too hot causes yellowing and brittleness. More is not always better.
For details see the material drying guide. If you have a moisture analyzer, measure instead of guessing; with splay this is the fastest reliable information.
Thermal degradation: temperature and residence time
If the material is dry but the air shot shows discoloration, the melt is getting too hot or staying too long in the barrel.
- Residence time in the barrel: if the shot volume is far below the barrel capacity (below about 20%), the material stays in the barrel for several cycles. Running a small mold on a large screw causes this. See Machine selection: shot volume and screw diameter
- Melt temperature: if you are at the upper end of the data sheet range, lower it in 10 °C steps.
- Screw speed and shear heat: high screw speed heats the melt above the heater setting. Reduce the speed so that recovery still fits within the cooling time.
- Dead spots: a worn check ring and dead corners in the nozzle or hot runner release degraded material intermittently. If the streaks appear now and then rather than every shot, look here.
- Additives and masterbatch: a masterbatch with an incompatible carrier or low thermal stability can release gas while the base material is fine. See Coloring with masterbatch
Trapped air: plasticizing settings
If the melt is clean but the streaks remain, the gas is most likely air that entered the screw during plasticizing.
- Too much decompression (suck-back): pulling the screw back at the end of recovery draws air in through the nozzle, and the next shot carries it into the cavity. Reduce decompression to the smallest value that still prevents drooling.
- Back pressure too low: the melt is not compacted enough and the air between pellets is not pushed out. Increase back pressure step by step.
- Feed zone too hot: pellets soften too early at the screw entry and the air cannot escape backwards. Check the feed zone setting and the feed throat cooling.
Causes on the mold side
- Condensation on the mold surface: a cold mold sweats in humid air. Streaks on the first shots or in summer point to this. Raise the mold temperature above the dew point or dry the air around the mold.
- Excessive shear at the gate: melt passing through a small gate at high speed heats up locally and degrades. If the streaks fan out right in front of the gate, try a larger gate or a lower initial injection speed.
- Oil, release agent and water leaks: water leaking into the cavity or too much release agent leaves the same mark. Streaks that always start at the same point indicate such a local source.
Recommended order
- Do an air shot and separate moisture, degradation or air.
- Measure the material moisture, or check the dryer's dew point, temperature and hopper residence time.
- Review melt temperature, screw speed and barrel residence time.
- Reduce decompression and increase back pressure.
- Check mold temperature, the gate area and any leaks into the cavity.
Change only one thing at a time and wait a few shots. To rank the causes by answering questions, use the defect diagnosis wizard.
Is something missing or wrong in this article? .